October 22, 2026

What Are The Common Annealing Processes?

Annealing is a metallurgical heat treatment process in which metal is slowly heated to a predetermined temperature, held (soaked) for a sufficient period, and then cooled at an appropriate rate.


1. Full Annealing

Used to refine coarse, overheated microstructures with poor mechanical properties in low- and medium-carbon steels after casting, forging, or welding.

  • Process: The workpiece is heated to 30–50 °C above the temperature where ferrite completely transforms into austenite (Ac_3), held for a specific soaking time, and then slowly cooled within the furnace. During cooling, austenite transforms again, resulting in a significantly refined grain structure.

2. Spheroidizing Annealing

Used to reduce excessive hardness in tool steels and bearing steels after forging, thereby improving machinability and cold-forming properties.

  • Process: The workpiece is heated to 20–40 °C above the temperature at which austenite begins to form (Ac_1), held at temperature, and then cooled slowly through the Ac_1 range. The lamellar cementite within the pearlite breaks down and spheroidizes into globular particles, effectively reducing material hardness. The same globular structure can also be produced by holding the steel for a long time just below Ac_1 (subcritical spheroidizing) or isothermally near Ac_1.

3. Isothermal Annealing

Used to lower the high hardness of medium- and high-carbon alloy structural steels and to improve their machinability.

  • Process: After austenitizing and soaking, the steel is rapidly cooled to a temperature just below Ac_1 (typically in the pearlite region, around 600–680 °C) where austenite is unstable, held isothermally until the austenite has fully transformed into pearlite (troostite or sorbite), and then cooled. Compared with full annealing, this produces a more uniform, lower hardness in a shorter cycle.

4. Recrystallization Annealing

Used to eliminate work-hardening effects (increased hardness and reduced ductility) in metal wire rods and sheets resulting from cold drawing or cold rolling.

  • Process: The workpiece is heated above its recrystallization temperature but below Ac_1 — typically 50–150 °C below the point where austenite begins to form (Ac_1). This eliminates strain-hardening effects, recrystallizes the deformed grain structure, and softens the metal.

5. Graphitization Annealing (Malleabilization)

Used to convert hard, brittle white cast iron (containing large amounts of cementite) into malleable cast iron with superior ductility.

  • Process: Castings are heated to approximately 950 °C, soaked for a designated period, and cooled at a controlled rate to decompose the cementite into flocculent graphite (temper carbon).

6. Diffusion Annealing (Homogenization Annealing)

Used to eliminate micro-segregation, homogenize chemical composition in alloy castings, and improve overall mechanical performance.

  • Process: Without inducing melting, the casting is heated to the highest feasible temperature below the solidus line — commonly 1,000–1,200 °C, depending on the grade — and soaked for an extended period (often several hours). Once the alloying elements have diffused uniformly through the matrix, the material is slowly cooled.

7. Stress-Relief Annealing

Used to eliminate residual stresses in steel castings, forgings, and welded structures.

  • Process: Steel components are heated to 100–200 °C below the lower critical temperature (Ac_1), soaked for a sufficient period, and then cooled slowly (large or complex parts should be furnace-cooled or still-air-cooled) to relieve internal stresses without causing a significant phase transformation.

Appendix

"Full Austenitization" Temperatures for Different Steel Types Although austenite begins to nucleate and grow right at the (Ac_1) temperature (around 727°C to 750°C), the steel must be heated to higher temperatures to allow its microstructure to fully and completely transform into austenite:

Steel Type Austenite Start Temperature Austenite Complete Temperature Description
Eutectoid Steel
(0.77% Carbon content)
(Ac_1) (Approx. 727°C) (Ac_1) (Approx. 727°C) Once the temperature crosses the critical point, the original pearlite transforms entirely into austenite immediately.
Hypoeutectoid Steel
(< 0.77% Carbon content, e.g., AISI 1045)
(Ac_1) (Approx. 730°C–750°C) (Ac_3) (Approx. 727°C–912°C; ≈780°C for AISI 1045) Pearlite transforms into austenite first upon reaching (Ac_1). The steel must be further heated past the (Ac_3) line for ferrite to disappear completely and become fully austenitic.
Hypereutectoid Steel
(> 0.77% Carbon content, e.g., Tool Steel)
(Ac_1) (Approx. 730°C–750°C) (Ac_{cm}) (Typically 750°C–950°C) Transformation begins at (Ac_1). The steel needs to be heated above the (Ac_{cm}) line to ensure secondary cementite completely dissolves into the austenite.